Top Banner
Root Defects. Internal Defects. Surface Defects. ه ش ی ر وب ی ع ی ن ا ی م وب ی ع ی ح ط س وب ی ع
30

Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

Jan 19, 2016

Download

Documents

Darrell Walters
Welcome message from author
This document is posted to help you gain knowledge. Please leave a comment to let me know what you think about it! Share it to your friends and learn new things together.
Transcript
Page 1: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

Root Defects. Internal Defects.Surface Defects.

عیوب ریشه عیوب میانی

عیوب سطحی

Page 2: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

از لحاظ نوع ایجاد تمرکز تنش

با اهمیت متوسط با اهمیت کم بااهمیت باال

1- 4 5 - 7 8- 10

EQUIAXED LINEAR VOLUMETRIC PLANAR Rounded and Slag lines Linear from at Non linear Elongated porosity least one

directionGas pores Slag inclusions Cracks, lack of

fusion

Page 3: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

INCOMPLETE ROOT PENETRATION.

LACK OF ROOT FUSION.

ROOT CONCAVITY.

BURN THROUGH.

EXCESS PENETRATION.

Page 4: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:Failure of weld metal to extend into the root of ajoint.CAUSES:Root faces too largeRoot gap too smallElectrode dia too largeIncorrect electrode angleArc length too longTravel speed too high forcurrent

عدم نفوذ پاس ریشه

Page 5: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:Lack of union at the root of the weld.

CAUSES:Amperage too low /

too highContaminated weld

preps

عدم ذوب ریشه

Page 6: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:A shallow groove that

mayoccur in the root of a

butt weld.

CAUSES:Root face too largeLow arc energyExcessive back purgeExcessive root

grinding

تقعر پاس ریشه

Page 7: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

نفوذ بیش از حد پاس ریشه

DEFINITION:Excessive weld metalprotruding through the root of a fusion weld

madefrom one side only.CAUSES:Excessive amperageExcessive root gapSmall root faceIncorrect welding techniqueType of electrode

Page 8: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:A localised collapse of the molten pool due to excessive penetration,resulting in a hole in the weld run.CAUSES:Excessive currentExcessive root grindingIncorrect welding technique

Page 9: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.
Page 10: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

LACK OF SIDE WALL FUSION.

LACK OF INTER RUN FUSION.

POROSITY.

SLAG INCLUSIONS.

Page 11: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:Lack of union in a

weld.

CAUSES:Contaminated weld

prepAmperage too low /

high

Page 12: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.
Page 13: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:A group of gas pores, formed by entrapped

gasduring the

solidificationof molten metal.Blowhole - a cavity generally over 1.5mm.Wormhole (piping) - elongated or tubular cavity.

Page 14: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.
Page 15: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:A fused, non-metallic residue produced from some processes.

CAUSES:Insufficient cleaningContaminationArc length too longWelding over irregularprofile

Page 16: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

ARC STRIKES.SURFACE CRACKS.SPATTER.POROSITY.EXCESS WELD METAL.CRATER PIPE.UNDERCUT. INCOMPLETELY FILLED GROOVE.OVERLAP.POOR WELD PROFILE.

Page 17: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:Damage on the parent material resulting from

the accidental striking of an arc from the weld.

CAUSES:Electrode straying intoparent materialElectrode holder Poor contact of return / earth clamp

Page 18: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:A linear discontinuity produced by fracture. Cracks may be longitudinal,transverse,edge, centreline, fusionzone, under bead, weld metal or parent metal.Weld metal cracks.Heat affected zone

cracksParent material/HAZ

Page 19: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:Small droplets of

electrodematerial which have strayed away from the arc which may or may

nothave fused to the

parent plate.CAUSES:Excessive arc energyArc - blowDamp electrodes

Page 20: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:A gas pore is a cavitygenerally under 1.5mm

india. Porosity is a group

ofgas pores.CAUSES:Moisture on prep / fluxContaminationArc length too longDamaged electrode fluxLoss of gas shield

Page 21: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.
Page 22: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:Additional weld metal, ateither the root or the

face,which may or may not be acceptable. Excess weld metal can cause a poor toe blend.CAUSES:Slow travel speedIncorrect welding

technique

Page 23: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:A depression due to shrinkage at the end

of a weld run, where the source of heat was removed.CAUSES:Deoxidation reactionLiquid to solid volume changeRapid cooling rate

Page 24: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:An irregular groove atthe toe of a weld runin the parent material,or in previously deposited weld metal, due to welding.CAUSES:Excessive welding

currentHigh welding speedWrong electrode angleExcessive weaving

Page 25: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:A continuous or intermittent channel in

the surface of a weld

running along its length, due to insufficient weld metal.CAUSES:Incorrect welding techniqueTravel speed too high

Page 26: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

The weld metals is in the under surface of base metals

Page 27: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:An imperfection at the

toe or root of a weld caused by metal flowing onto the surface of the parent

plate without fusing to it.CAUSES:ContaminationSlow travel speedHigh amperageWelding technique

Page 28: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.
Page 29: Root Defects. Internal Defects. Surface Defects. عیوب ریشه عیوب میانی عیوب سطحی.

DEFINITION:A non uniform/irregularappearance at either the weld face or root. Can include excessive

rootpenetration/cap heightand poor cap profile.CAUSES:Poor welding technique.Too slow/fast travel

speedArc blow