Investigation on the mechanism responsible for degradation on Cu/ Kapton foils . Andy Wu. The degraded Foil . SEM Images of Spot A. SEM Image of Part of Spot B. EDX Observations at 25kV (A). Typical Spectrum for Spots A and B . Typical EDX Spectrum at 25kV (open window). - PowerPoint PPT Presentation
Welcome message from author
This document is posted to help you gain knowledge. Please leave a comment to let me know what you think about it! Share it to your friends and learn new things together.
Transcript
Page 1: Investigation on the mechanism responsible for degradation on Cu/ Kapton  foils

Investigation on the mechanism responsible for degradation on Cu/Kapton foils

Andy Wu

Page 2: Investigation on the mechanism responsible for degradation on Cu/ Kapton  foils

The degraded Foil

Page 3: Investigation on the mechanism responsible for degradation on Cu/ Kapton  foils

SEM Images of Spot A

Page 4: Investigation on the mechanism responsible for degradation on Cu/ Kapton  foils

SEM Image of Part of Spot B

Page 5: Investigation on the mechanism responsible for degradation on Cu/ Kapton  foils

EDX Observations at 25kV (A)

Typical Spectrum for Spots A and B

Page 6: Investigation on the mechanism responsible for degradation on Cu/ Kapton  foils

Typical EDX Spectrum at 25kV (open window)

Typical Open Window Spectrum for Spots A&B

Page 7: Investigation on the mechanism responsible for degradation on Cu/ Kapton  foils

Typical EDX Spectrum at 10 KV (surface)

Typical Open Window Spectrum at 10 kV for Spots A&B

Page 8: Investigation on the mechanism responsible for degradation on Cu/ Kapton  foils

Conclusion

• The surfaces of the degraded spots are covered by a thin layer of copper oxides. The thickness of the layer is much below 1 μm.

Page 9: Investigation on the mechanism responsible for degradation on Cu/ Kapton  foils

Composition of Granite

SiO 72.04%, Al2O3 14.42%, K2O 4.12%, Na2O 3.69%, CaO 1.82%, FeO 1.68%, Fe2O3 1.22%, MgO 0.71%, TiO2 0.30%, P2O5 0.12%, MnO 0.05%

Page 10: Investigation on the mechanism responsible for degradation on Cu/ Kapton  foils

Possible degradation mechanism

• Evaporation of the DI water used to mediate the contact between Cu/Kapton foil and granite leads to several highly localized small area where active oxygen can reach certain level to be reactive to Cu. The active oxygen can come either from granite or possible residues from the manufacturer as one can see that the surface of the as received foil has discolored spots.

Page 11: Investigation on the mechanism responsible for degradation on Cu/ Kapton  foils

Recommended Remedy

• Seal the granite table to prevent the formation of some localized water spots.

• Ask the manufacturer to do a better job on cleaning the Cu/Kapton foils