Laporan Tugas Akhir Kinerja Kuat Lentur Pada Balok Beton Dengan Pengekangan Jaring- Jaring Nylon dan Expanded Metal Andri lelono 07.12.0038 Ida Bagus W.D 04.12.0032 L-9 HASIL PERHITUNGAN PENGUJIAN BERAT JENIS SEMEN Suhu Awal : 25°C Semen : 64 gram Piknometer I A. Berat semen : 64 gram B. Volume I zat cair : 0,2 ml C. Volume II zat cair : 18,5 ml D. Berat isi air : 1 gr/cm 3 Berat jenis Semen = D B C A × − = 1 2 , 0 5 , 18 64 × − = 3,49 gr/cm 3 Piknometer I A. Berat semen : 64 gram B. Volume I zat cair : 1,1 ml C. Volume II zat cair : 19,5 ml D. Berat isi air : 1 gr/cm 3 Berat jenis Semen = D B C A × − = 1 1 , 1 5 , 19 64 × − = 3,47 gr/cm 3 Berat jenis rata-rata : 2 47 , 3 49 , 3 + = 3,48 gr/cm 3
21
Embed
HASIL PERHITUNGAN PENGUJIAN BERAT JENIS SEMENrepository.unika.ac.id/4695/6/04.12.0032 Ida Bagus... · Kinerja Kuat Lentur Pada Balok Beton Dengan Pengekangan Jaring- Jaring Nylon
This document is posted to help you gain knowledge. Please leave a comment to let me know what you think about it! Share it to your friends and learn new things together.
Transcript
Laporan Tugas Akhir Kinerja Kuat Lentur Pada Balok Beton Dengan Pengekangan Jaring- Jaring Nylon dan Expanded Metal
Andri lelono 07.12.0038 Ida Bagus W.D 04.12.0032 L-9
HASIL PERHITUNGAN
PENGUJIAN BERAT JENIS SEMEN
Suhu Awal : 25°C Semen : 64 gram Piknometer I
A. Berat semen : 64 gram B. Volume I zat cair : 0,2 ml C. Volume II zat cair : 18,5 ml D. Berat isi air : 1 gr/cm3
Berat jenis Semen = DBC
A×
−
= 12,05,18
64×
−
= 3,49 gr/cm3 Piknometer I
A. Berat semen : 64 gram B. Volume I zat cair : 1,1 ml C. Volume II zat cair : 19,5 ml D. Berat isi air : 1 gr/cm3
Berat jenis Semen = DBC
A×
−
= 11,15,19
64×
−
= 3,47 gr/cm3
Berat jenis rata-rata : 2
47,349,3 + = 3,48 gr/cm3
Laporan Tugas Akhir Kinerja Kuat Lentur Pada Balok Beton Dengan Pengekangan Jaring- Jaring Nylon dan Expanded Metal
Andri lelono 07.12.0038 Ida Bagus W.D 04.12.0032 L-9
HASIL PERHITUNGAN
PENGUJIAN KONSISTENSI NORMAL SEMEN
Berat Semen : 300 gram Ø Jarum Vicat : 10 mm Suhu : 27°C Air (%)
PENURUNAN TIAP 30 DETIK (mm)
25 17 26 22 27 30 28 42 29 45 30 48
Perhitungan prosentase air :
a. 25 % → ccgrgr 757530010025
≈=×
b. 26 % → ccgrgr 787830010026
≈=×
c. 27 % → ccgrgr 818130010027
≈=×
d. 28 % → ccgrgr 848430010028
≈=×
e. 29 % → ccgrgr 878730010029
≈=×
f. 30 % → ccgrgr 909030010030
≈=×
Laporan Tugas Akhir Kinerja Kuat Lentur Pada Balok Beton Dengan Pengekangan Jaring- Jaring Nylon dan Expanded Metal
Andri lelono 07.12.0038 Ida Bagus W.D 04.12.0032 L-9
HASIL PERHITUNGAN
PENGUJIAN KONSISTENSI NORMAL SEMEN
Berat Semen : 300 gram Ø Jarum Vicat : 1 mm Prosentase Air : 27 %
Jumlah Air : ccgrgr 818130010027
≈=×
WAKTU PENURUNAN AIR (Menit)
PENURUNAN TIAP 15 MENIT (mm)
0 42 15 32 30 28 45 24 60 21
Laporan Tugas Akhir Kinerja Kuat Lentur Pada Balok Beton Dengan Pengekangan Jaring- Jaring Nylon dan Expanded Metal
Andri lelono 07.12.0038 Ida Bagus W.D 04.12.0032 L-9
HASIL PERHITUNGAN
PENGUJIAN BERAT VOLUME AGREGAT KASAR dan HALUS
Agregat Kasar
A. Volume Wadah = 3,00063 liter B. Berat Wadah = 4,3 kg C. Berat Wadah + Benda uji = 8,5 kg D. Berat Benda Uji (C-B) = 8,5 – 4,3 = 4,2 kg
Berat Volume (D/A) = 3,42,4 = 0,976 kg/liter
Agregat Halus A. Volume Wadah = 3,00263 liter B. Berat Wadah = 4,3 kg C. Berat Wadah + Benda uji = 8,7 kg D. Berat Benda Uji (C-B) = 8,7 – 4,3 = 4,4 kg
Berat Volume (D/A) = 3,44,4 = 1,023 kg/liter
Laporan Tugas Akhir Kinerja Kuat Lentur Pada Balok Beton Dengan Pengekangan Jaring- Jaring Nylon dan Expanded Metal
Andri lelono 07.12.0038 Ida Bagus W.D 04.12.0032 L-9
HASIL PERHITUNGAN PENGUJIAN KADAR AIR AGREGAT KASAR dan HALUS
Agregat Kasar
A. Berat Wadah = 0,150 kg B. Berat Wadah + Benda uji = 3,15 kg C. Berat Benda Uji (B-A) = 3 kg D. Berat Benda Uji Kering = 2,95 kg
E. Kadar Air %100×−D
DC = %69,1%10095,2
95,23=×
−
Agregat Halus
A. Berat Wadah = 0,150 kg B. Berat Wadah + Benda uji = 0,650 kg C. Berat Benda Uji = 0,5 kg D. Berat Benda Uji Kering = 0,43 kg
E. Kadar Air %100×−D
DC = %28,16%10043,0
43,05,0=×
−
Laporan Tugas Akhir Kinerja Kuat Lentur Pada Balok Beton Dengan Pengekangan Jaring- Jaring Nylon dan Expanded Metal
Andri lelono 07.12.0038 Ida Bagus W.D 04.12.0032 L-9
HASIL PERHITUNGAN
PENGUJIAN ANALISA SPECIFIC GRAFITY
dan PENYERAPAN AGREGAT KASAR
A. Berat contoh SSD = 1200 gram B. Berat contoh dalam air = 653 gram C. Berat contoh kering udara = 1015 gram
Apparent Specific Grafity = BC
C−
= 84,26531015
1015=
−
Bulk Specific Grafity kondisi kering = BA
C−
= 87,16531200
1015=
−
Bulk Specific Grafity kondisi SSD = BA
A−
= 19,26531200
1200=
−
% Penyerapan Air = %100×−A
CA = %20,18%1001015
10151200=×
−
Laporan Tugas Akhir Kinerja Kuat Lentur Pada Balok Beton Dengan Pengekangan Jaring- Jaring Nylon dan Expanded Metal
Andri lelono 07.12.0038 Ida Bagus W.D 04.12.0032 L-9
HASIL PERHITUNGAN PENGUJIAN ANALISA SPECIFIC GRAFITY
dan PENYERAPAN AGREGAT HALUS
A. Berat Piknometer = 172 gram B. Berat contoh SSD = 500 gram C. Berat contoh dalam air = 980 gram D. Berat contoh kering udara = 708 gram E. Berat contoh kering = 493,2gram
Apparent Specific Grafity =CDE
E−+
= 22,29807082,493
2,493=
−+
Bulk Specific Grafity kondisi kering =CDB
E−+
= 16,2980708500
2,493=
−+
Bulk Specific Grafity kondisi SSD =CDB
B−+
= 19,2980708500
500=
−+
% Penyerapan Air = %100×−E
EB = %38,1%1002,493
2,493500=×
−
Laporan Tugas Akhir Kinerja Kuat Lentur Pada Balok Beton Dengan Pengekangan Jaring- Jaring Nylon dan Expanded Metal
Andri lelono 07.12.0038 Ida Bagus W.D 04.12.0032 L-9