Y x Z section X RESULT With applying load W, the specimen will sustain a stress. At point O, M = 0 ∑ 500 x W = F x 50 F = 10 W Where F = the actual load will apply on the specimen, N Creep specimen Y = width Z = thickness 500 mm 50 mm Specime n W, load
This document is posted to help you gain knowledge. Please leave a comment to let me know what you think about it! Share it to your friends and learn new things together.
Transcript
Y x Z section
X
RESULT
With applying load W, the specimen will sustain a stress.
At point O,
∑M = 0
500 x W = F x 50
F = 10 W
Where F = the actual load will apply on the specimen, N
Creep specimen
Y = width
Z = thickness
500 mm50 mm
Specimen
W, load
Table 1
Length, mm
Experiment 1 31.91
Thickness,
mm5.050
Width, mm 5.050
Experiment 2 28.50
Thickness,
mm5.027
Width, mm 5.027
Experiment 3 31.91
Thickness,
mm5.090
Width, mm 5.090
Experiment 4 31.60
Thickness,
mm5.084
Width, mm 5.084
Experiment 1 : ( Table 2 )
Temperature : 80 ⁰C
Load : 2 N
Time ( minute ) Deflection ( mm )
0 1.91
1 2.10
2 2.29
3 2.42
4 2.48
5 2.56
6 2.61
7 2.64
8 2.69
Calculation :
Specimen cross section area :
(A) = Y x Z
(A) = 5.050 mm x 5.050 mm
=25.50 mm²
Stress act on the specimen :
(σ) = F/A = 10 W/A
(σ) = 2N / 25.50 mm²
= 0.08 N / mm²
Creep strain:
(ϵ ) = elongation of current time / original length
= L’ / x
Experiment 1 : ( Table 3 )
Temperature : 80 ⁰C
Load : 2 N
Time ( minute ) Deflection ( mm ) Length,L0 (mm) Creep Strain,ε
0 1.91 31.91 0.060
1 2.10 31.91 0.066
2 2.29 31.91 0.072
3 2.42 31.91 0.076
4 2.48 31.91 0.078
5 2.56 31.91 0.080
6 2.61 31.91 0.082
7 2.64 31.91 0.083
8 2.69 31.91 0.084
Time (minute ) = 0
1.91 mm / 31.91 mm = 0.060 mm
Time (minute ) = 1
2.10mm /31.91 mm = 0.066mm
Time (minute ) = 2
2.29mm / 31.91mm = 0.072 mm
Time (minute ) = 3
2.42mm / 31.91mm = 0.076 mm
Time (minute ) = 4
2.48mm / 31.91mm = 0.078 mm
Time (minute ) = 5
2.56mm / 31.91mm = 0.080 mm
Time (minute ) = 6
2.61mm / 31.91mm = 0.082 mm
Time (minute ) = 7
2.64mm /31.91 mm = 0.083 mm
Time (minute ) = 8
2.69mm / 31.91mm = 0.084mm
Modulus of elasticity :
(E) = stress / strain
= σ / ϵ
Stress, N / mm² Creep Strain,ε Modulus of elasticity, (E)
0.08 0.060 1.33
0.08 0.066 1.21
0.08 0.072 1.11
0.08 0.076 1.05
0.08 0.078 1.02
0.08 0.080 1.00
0.08 0.082 0.98
0.08 0.083 0.96
0.08 0.084 0.95
Time (minute ) = 0 Time (minute ) = 1
0.08 / 0.060 =1.33 N / mm 0.08 / 0.066 = 1.21 N / mm
Time (minute ) = 2 Time (minute ) = 3
0.08 / 0.072 = 1.11 N / mm 0.08 / 0.076 = 1.05 N / mm
Time (minute ) = 4 Time (minute ) = 5
0.08 / 0.078 = 1.02 N / mm 0.08 / 0.080 = 1.00N / mm
Time (minute ) = 6 Time (minute ) = 7
0.08 / 0.082 = 0.98 N / mm 0.08 / 0.083 = 0.96 N / mm
Time (minute ) = 8
0.08 / 0.084 = 0.95 N / mm
Experiment 2 : ( Table 4 )
Temperature : 100 ⁰C
Load : 2 N
Time ( minute ) Deflection ( mm )
0 4.38
1 5.40
2 5.90
3 6.10
4 6.38
5 6.52
6 6.66
7 6.91
8 7.14
Calculation :
Specimen cross section area :
(B) = Y x Z
(B) = 5.027 mm x 5.027 mm
= 25.27 mm²
Stress act on the specimen :
(σ) = F/A = 10 W/A
(σ) = 2N /25.27 mm²
= 0.08 N / mm²
Creep strain:
(ϵ ) = elongation of current time / original length
= L’ / x
Experiment 2 : ( Table 5 )
Temperature : 100 ⁰C
Load : 2 N
Time ( minute ) Deflection ( mm ) Length,L0 (mm) Creep Strain,ε
0 4.38 28.50 0.154
1 5.40 28.50 0.189
2 5.90 28.50 0.207
3 6.10 28.50 0.214
4 6.38 28.50 0.224
5 6.52 28.50 0.229
6 6.66 28.50 0.234
7 6.91 28.50 0.242
8 7.14 28.50 0.251
Time (minute ) = 0
4.38 mm / 28.50 mm = 0.154 mm
Time (minute ) = 1
5.40 mm / 28.50 mm = 0.189 mm
Time (minute ) = 2
5.90 mm / 28.50 mm = 0.207 mm
Time (minute ) = 3
6.10 mm / 28.50 mm = 0.214 mm
Time (minute ) = 4
6.38 mm / 28.50 mm = 0.224 mm
Time (minute ) = 5
6.52 mm / 28.50 mm = 0.229mm
Time (minute ) = 6
6.66 mm / 28.50 mm = 0.234 mm
Time (minute ) = 7
6.91 mm / 28.50 mm = 0.242 mm
Time (minute ) = 8
7.14 mm / 28.50 mm = 0.251 mm
Modulus of elasticity :
(E) = stress / strain
= σ / ϵ
Stress, N / mm² Creep Strain,ε Modulus of elasticity, (E)
0.08 0.154 0.519
0.08 0.189 0.423
0.08 0.207 0.386
0.08 0.214 0.374
0.08 0.224 0.357
0.08 0.229 0.349
0.08 0.234 0.342
0.08 0.242 0.331
0.08 0.251 0.319
Time (minute ) = 0 Time (minute ) = 1
0.08/ 0.154 =0.519 N / mm 0.08 /0.189 = 0.423 N / mm
Time (minute ) = 2 Time (minute ) = 3
0.08/0.207 = 0.386 N / mm 0.08 / 0.214 = 0.374N / mm
Time (minute ) = 4 Time (minute ) = 5
0.08 / 0.224 = 0.357 N / mm 0.08 / 0.229 =0.349N / mm
Time (minute ) = 6 Time (minute ) = 7
0.08 / 0.234 = 14.29 N / mm 0.08 /0.242=0.331 N / mm
Time (minute ) = 8
0.08 / 0.251 = 0.319 N / mm
Experiment 3 : ( Table 7 )
Temperature : 80 ⁰C
Load : 3 N
Time ( minute ) Deflection ( mm )
0 2.90
1 3.55
2 4.30
3 6.10
4 6.99
5 7.30
6 7.32
7 7.34
8 7.38
Calculation :
Specimen cross section area :
(C) = Y x Z
(C) = 5.09 mm x 5.09 mm
= 25,91 mm²
Stress act on the specimen :
(σ) = F/A = 10 W/A
(σ) = 3N / 25.91 mm²
= 0.12N / mm²
Creep strain:
(ϵ ) = elongation of current time / original length
= L’ / x
Experiment 3 : ( Table 8 )
Temperature : 80 ⁰C
Load : 3 N
Time ( minute ) Deflection ( mm ) Length,L0 (mm) Creep Strain,ε
0 2.90 31.91 0.091
1 3.55 31.91 0.111
2 4.30 31.91 0.135
3 6.10 31.91 0.191
4 6.99 31.91 0.219
5 7.30 31.91 0.229
6 7.32 31.91 0.229
7 7.34 31.91 0.230
8 7.38 31.91 0.231
Time (minute ) = 0
2.90 mm / 31.91 mm = 0.091 mm
Time (minute ) = 1
3.55mm / 31.91 mm = 0.111 mm
Time (minute ) = 2
4.30 mm / 31.91 mm = 0.135 mm
Time (minute ) = 3
6.10 mm / 31.91 mm = 0.191 mm
Time (minute ) = 4
6.99 mm / 31.91 mm = 0.219 mm
Time (minute ) = 5
7.30 mm / 31.91 mm = 0.229 mm
Time (minute ) = 6
7.32 mm / 31.91 mm = 0.229 mm
Time (minute ) = 7
7.34 mm / 31.91 mm = 0.0.230 mm
Time (minute ) = 8
7.38 mm / 31.91 mm = 0.231 mm
Modulus of elasticity :
(E) = stress / strain
= σ / ϵ
Stress, N / mm² Creep Strain,ε Modulus of elasticity, (E)
0.12 0.091 1.319
0.12 0.111 1.081
0.12 0.135 0.889
0.12 0.191 0.628
0.12 0.219 0.548
0.12 0.229 0.524
0.12 0.229 0.524
0.12 0.230 0.522
0.12 0.231 0.519
Time (minute ) = 0 Time (minute ) = 1
0.12 / 0.091 =1.319 N / mm 0.12/ 0.111=1.081 N / mm
Time (minute ) = 2 Time (minute ) = 3
0.12/ 0.135 = 0.889 N / mm 0.12/ 0.191 = 0.628 N / mm
Time (minute ) = 4 Time (minute ) = 5
0.12 / 0.219 = 0.548 N / mm 0.12 / 0.229 = 0.524 N / mm
Time (minute ) = 6 Time (minute ) = 7
0.12 / 0.229 = 0.524 N / mm 0.12 / 0.230 = 0.522 N / mm
Time (minute ) =
0.12 /0.231 = 0.519 N / mm
Experiment 4 : ( Table 9 )
Temperature : 100 ⁰C
Load : 3 N
Time ( minute ) Deflection ( mm )
0 4.90
1 6.22
2 7.30
3 7.34
4 7.42
5 7.50
6 7.54
7 7.60
8 7.63
Calculation :
Specimen cross section area :
(D) = Y x Z
(D) = 5.084 mm x 5.084 mm
= 25.85 mm²
Stress act on the specimen :
(σ) = F/A = 10 W/A
(σ) = 3N / 25.85 mm²
= 0.12 N / mm²
Creep strain:
(ϵ ) = elongation of current time / original length
= L’ / x
Experiment 4 : ( Table 10 )
Temperature : 100 ⁰C
Load : 3 N
Time ( minute ) Deflection ( mm ) Length,L0 (mm) Creep Strain,ε
0 4.90 31.60 0.155
1 6.22 31.60 0.197
2 7.30 31.60 0.231
3 7.34 31.60 0.232
4 7.42 31.60 0.235
5 7.50 31.60 0.237
6 7.54 31.60 0.239
7 7.60 31.60 0.241
8 7.63 31.60 0.241
Time (minute ) = 0
4.90 mm / 31.60 mm = 0.155 mm
Time (minute ) = 1
6.22mm / 31.60 mm = 0.197 mm
Time (minute ) = 2
7.30 mm / 31.60 mm = 0.231 mm
Time (minute ) = 3
7.34 mm / 31.60 mm = 0.232 mm
Time (minute ) = 4
7.42 mm / 31.60 mm = 00.235 mm
Time (minute ) = 5
7.50 mm / 31.60 mm = 0.237mm
Time (minute ) = 6
7.54 mm / 31.60 mm = 0.239 mm
Time (minute ) = 7
7.60 mm / 31.60 mm = 0.241 mm
Time (minute ) = 8
7.63 mm / 31.60 mm = 0.241 mm
Modulus of elasticity :
(E) = stress / strain
= σ / ϵ
Stress, N / mm² Creep Strain,ε Modulus of elasticity, (E)
0.12 0.155 0.774
0.12 0.197 0.609
0.12 0.231 0.519
0.12 0.232 0.517
0.12 0.235 0.511
0.12 0.237 0.506
0.12 0.239 0.502
0.12 0.241 0.498
0.12 0.241 0.498
Time (minute ) = 0 Time (minute ) = 1
0.12/ 0.155 =0.774 N / mm 0.12 / 0.197 = 0.609 N / mm
Time (minute ) = 2 Time (minute ) = 3
0.12/ 0.231 = 0.519 N / mm 0.12 / 0.232 = 0.517 N / mm
Time (minute ) = 4 Time (minute ) = 5
0.12 / 0.235 = 0.511 N / mm 0.12 / 0.237 = 0.506 N / mm
Time (minute ) = 6 Time (minute ) = 7
0.12 / 0.239 = 0.502 N / mm 0.12 / 0.241 =0.498 N / mm
Time (minute ) = 8
0.12 / 0.241 = 0.498 N / mm
GRAF
0 1 2 3 4 5 6 7 80
0.01
0.02
0.03
0.04
0.05
0.06
0.07
0.08
0.09
Creep Strain vs Time curves for exp. 1
Time(minute)
Cree
p S
trai
n
0 1 2 3 4 5 6 7 80
0.05
0.1
0.15
0.2
0.25
0.3
Creep Strain vs Time Curves for exp.2
Time(minute)
Cre
ep s
trai
n
0 1 2 3 4 5 6 7 80
0.05
0.1
0.15
0.2
0.25
Creep Strain vs Time Curves for exp.3
Time(minute)
Cree
p St
rain
DISCUSSIONS
0 1 2 3 4 5 6 7 80
0.05
0.1
0.15
0.2
0.25
0.3
Creep Strain vs Time Curves for exp. 4
Time(minute)
Cree
p S
trai
n
Creep is high temperature progressive deformation at constant stress. "High
temperature" is a relative term dependent upon the materials involved. Creep rates are used in
evaluating materials for boilers, gas turbines, jet engines, ovens, or any application that
involves high temperatures under load. Understanding high temperature behaviour of metals
is useful in designing failure resistant systems.
When a material like steel is plastically deformed at ambient temperatures its strength
is increased due to work hardening. This work hardening effectively prevents any further
deformation from taking place if the stress remains approximately constant. Annealing the
deformed steel at an elevated temperature removes the work hardening and restores the steel
to its original condition.
However, if the steel is plastically deformed at an elevated temperature, then both
work hardening and annealing take place simultaneously. A consequence of this is that steel
under a constant stress at an elevated temperature will continuously deform with time, that is,
it is said to "creep”.
To determine creep properties, material is subjected to prolonged constant tension or
compression loading at constant temperature. Deformation is recorded at specified time
intervals and a creep vs. time diagram is plotted. Slope of curve at any point is creep rate. If
failure occurs, it terminates test and Time for Rupture is recorded.
Like the Creep Test, Stress Rupture Testing involves a tensile specimen under a
constant load at a constant temperature. The difference being, Stress Rupture Testing uses
higher stresses and is always continued until failure of the material occurs. The Stress
Rupture test is used to determine the time to failure and elongation.
If specimen does not fracture within test period, creep recovery may be measured. To
determine stress relaxation of material, specimen is deformed a given amount and decrease in
stress over prolonged period of exposure at constant temperature is recorded. Standard creep
testing procedures are detailed in ASTM E-139, ASTM D-2990 and D-2991 (plastics) and
ASTM D-2294 (adhesives).
A creep test involves a tensile specimen under a constant load maintained at a
constant temperature. Measurements of strain are then recorded over a period of time. Creep
occurs in three stages: Primary, or Stage I; Secondary, or Stage II: and Tertiary, or Stage III.
Stage I, or Primary creep occurs at the beginning of the tests, and creep is mostly transiently,
not at a steady rate.
Resistance to creep increases until Stage II is reached. In Stage II, or Secondary
creep, the rate of creep becomes roughly steady. This stage is often referred to as steady state
creep. In Stage III, or tertiary creep, the creep rate begins to accelerate as the cross sectional
area of the specimen decreases due to necking or internal voiding decreases the effective area
of the specimen. If stage III is allowed to proceed, fracture will occur.
The creep test is usually employed to determine the minimum creep rate in Stage II.
Engineers need to account for this expected deformation when designing systems. A creep
test is carried out by applying a constant load to a specimen and observing the increase in