Atomic Layer Deposition of Metal Fluorides Using HF ...€¦ · deposition (PVD) methods. These PVD methods include sputtering,12,13 thermal evaporation,14−16 electron beam deposition,1,17
This document is posted to help you gain knowledge. Please leave a comment to let me know what you think about it! Share it to your friends and learn new things together.
Transcript
Atomic Layer Deposition of Metal Fluorides Using HF−Pyridine asthe Fluorine PrecursorYounghee Lee,† Huaxing Sun,† Matthias J. Young,‡ and Steven M. George*,†,§
†Department of Chemistry and Biochemistry, ‡Department of Chemical and Biological Engineering, and §Department of MechanicalEngineering, University of Colorado, Boulder, Colorado 80309, United States
*S Supporting Information
ABSTRACT: The atomic layer deposition (ALD) of a variety ofmetal fluorides including ZrF4, MnF2, HfF4, MgF2, and ZnF2 wasdemonstrated using HF from a HF−pyridine solution. In situquartz crystal microbalance (QCM) studies were utilized toexamine the growth of these metal fluorides. ZrF4 ALD usingtetrakis(ethylmethylamido) zirconium and HF as the reactants wasstudied as a model system. The QCM measurements determined amass gain per cycle (MGPC) of 35.5 ng/(cm2 cycle) for ZrF4 ALDat 150 °C. This MGPC was equivalent to a growth rate of 0.9 Å/cycle at 150 °C. MnF2, HfF4, MgF2, ZnF2, and additional ZrF4were also grown using bis(ethylcyclopentadienyl) manganese,tetrakis(dimethylamido) hafnium, bis(ethylcyclopentadienyl) mag-nesium, diethylzinc, and zirconium tetra-tert-butoxide as the metalprecursors, respectively. The growth rates for MnF2, HfF4, MgF2,ZnF2, and ZrF4 ALD were 0.4, 0.8, 0.4, 0.7, and 0.6 Å/cycle, respectively, at 150 °C. All of these metal fluoride ALD systemsdisplayed self-limiting reactions. Ex situ measurements of the growth rates using X-ray reflectivity and spectroscopic ellipsometryanalysis agreed with the in situ QCM measurements. Analysis of the QCM mass changes after the individual metal precursor andHF exposures quantified HF adsorption after the HF reaction. The ZrF4 and HfF4 films acted as strong Lewis acids and adsorbedan average of two HF per deposited MFy species after the HF reaction. In contrast, the MnF2, MgF2, and ZnF2 films all behavedas weak Lewis acids and did not adsorb HF after the HF reaction. The refractive indices of the metal fluoride films were inagreement with previous optical measurements. Most of the metal fluoride films were crystalline as measured by X-ray diffractionstudies. The majority of the metal fluoride films also had high purity as established by X-ray photoelectron spectroscopy studies.This pathway for metal fluoride ALD using HF−pyridine as the fluorine precursor will be useful for many applications of metalfluoride films such as optical coatings in the ultraviolet wavelength region.
I. INTRODUCTION
Metal fluorides are important optical coating materials becausethey have a low refractive index and high transmission atultraviolet (UV) and infrared (IR) wavelengths.1−3 Some metalfluorides also have strong Lewis acidity and are used asheterogeneous catalysts for the manufacture of chlorofluor-ocarbons (CFCs).4−6 Various metal fluorides, such as AlF3, arealso useful protective coatings on Li ion battery electrodes.7,8 Inaddition, metal fluorides are known to be important surfacereaction intermediates during thermal atomic layer etching(ALE).9−11
Metal fluoride films can be deposited using physical vapordeposition (PVD) methods. These PVD methods includesputtering,12,13 thermal evaporation,14−16 electron beamdeposition,1,17 and ion-assisted deposition.18,19 Atomic layerdeposition (ALD) methods can also be employed to growmetal fluorides. ALD is a technique that deposits extremelyconformal and continuous thin films with atomic level controlusing sequential, self-limiting surface reactions.20 In general,metal fluoride ALD has been difficult because the HF precursor
is dangerous and corrosive. Consequently, the ALD of mostmetal fluorides has been performed using other fluorineprecursors than HF.The first demonstration of metal fluoride ALD reported
CaF2, SrF2, and ZnF2 ALD using NH4F solid as the fluorinesource.21 NH4F was delivered by sublimation at 80 °C into thereactor. The NH4F decomposed to NH3 and HF at reactiontemperatures between 260 and 400 °C.21 The ALD ofMgF2,
22,23 LaF3,24 YF3,
25 and LiF26 has been demonstratedusing either TiF4 or TaF5 as the fluorine source. The ligandexchange between metal 2,2,6,6-tetramethyl-3,5-heptanedionate(M(tmhd)x) and TiF4 or TaF5 yields the metal fluoride (MFy)layer and volatile Ti(tmhd)4 or Ta(tmhd)5 as a byproduct.MgF2 ALD has also been performed using anhydrous HFderived from a gas cylinder.27 Hexafluoroacetylacetonate as the
Received: November 9, 2015Revised: February 26, 2016Published: March 1, 2016
fluorine source together with ozone has also been used to growMgF2, CaF2, and LaF3 ALD films.28
We initially described AlF3 ALD with trimethylaluminum(TMA) and HF from a HF−pyridine solution.29,30 The HF−pyridine solution consists of 70% HF and 30% pyridine and iscommonly referred to as Olah’s reagent.31 HF−pyridine is aliquid at room temperature and is in equilibrium with gaseousHF. Recent measurements have reported a HF vapor pressureof 90−100 Torr over HF−pyridine solutions.10 Massspectrometer experiments have also not detected measurablepyridine in the vapor above HF−pyridine solutions.30 HF fromHF−pyridine solutions avoids the problems of using HF fromcompressed gas cylinders and provides a safer alternative toanhydrous HF.In this paper, the ALD of various metal fluorides was
demonstrated using a variety of metal precursors and HFderived from HF−pyridine as the fluorine precursor. The metalprecursors, tetrakis(ethylmethylamido) zirconium, bis-(ethylcyclopentadienyl) manganese, tetrakis(dimethylamido)hafnium, bis(ethylcyclopentadienyl) magnesium, diethylzinc,and zirconium tetra-tert-butoxide, were employed for the ALDof ZrF4, MnF2, HfF4, MgF2, ZnF2, and ZrF4, respectively. Themetal fluoride ALD was studied using in situ quartz crystalmicrobalance (QCM) investigations at 150 °C.The thickness and density of metal fluoride ALD films were
derived using ex situ X-ray reflectivity (XRR) analysis. Inaddition, the film thickness and refractive index of the metalfluorides were obtained using spectroscopic ellipsometry (SE).The composition and structure of the metal fluoride ALD filmswere also determined with X-ray photoelectron spectroscopy(XPS) and grazing incidence X-ray diffraction (GIXRD)analysis. These results should be useful for the growth andapplication of metal fluoride ALD films.
II. EXPERIMENTAL SECTIONII.I. Viscous Flow Reactor with in Situ QCM. The ALD reactions
were conducted in a viscous flow reactor containing the in situ quartzcrystal microbalance (QCM) at 150 °C.32,33 A mechanical pump(Pascal 2015SD, Alcatel) provided vacuum conditions in the ALDreactor. The reactants were transported through the reactor using a N2carrier gas. Mass flow controllers (Type 1179A, MKS) delivered aconstant N2 carrier gas flow at 150 sccm. This N2 gas flow and thepumping established a base pressure of ∼1 Torr in the reactor. Thereactor was maintained at a fixed temperature within ±0.04 °C using aPID temperature controller (2604, Eurotherm). Pressure changes weremonitored during the reactions using a bakeable capacitancemanometer (Baratron 121A, MKS).The metal fluoride ALD reactions were conducted using various
metal precursors. These metal precursors were tetrakis-(ethylmethylamido) zirconium (TEMAZ, 99.99%, Sigma-Aldrich,),bis(ethylcyclopentadienyl) manganese (Mn(EtCp)2, 98%, Strem),tetrakis(dimethylamido) hafnium (TDMAH, 99.99%, Sigma-Aldrich),bis(ethylcyclopentadienyl) magnesium (Mg(EtCp)2, 98%, Strem),diethylzinc (DEZ, Zn 52.0%, Sigma-Aldrich), and zirconium tetra-tert-butoxide (ZTB, 99%, Strem). The molecular structures of thevarious metal precursors are illustrated in Figure 1. The bubblertemperatures for TEMAZ, Mn(EtCp)2, TDMAH, Mg(EtCp)2, andZTB were held at 112, 100, 67, 92, and 65 °C, respectively. The DEZprecursor was maintained at room temperature.Each metal fluoride ALD experiment was performed on a fresh
metal oxide ALD film that was grown at 150 °C. The initial metaloxide ALD films were prepared using the same metal precursors asemployed for the metal fluoride ALD. H2O (Chromasolv for HPLC,Sigma-Aldrich) was used as the reactant for the metal oxide ALD.HF−pyridine solution (70 wt % HF, Sigma-Aldrich) was contained ina gold-plated stainless steel bubbler and was transferred to this bubbler
in a dry N2-filled glovebag. The HF−pyridine and H2O precursorswere at room temperature.
The in situ QCM measurements were performed using a filmdeposition monitor (Maxtek TM-400, Inficon). The QCM sensorswere 6 MHz, AT-cut (Colorado Crystal Corp.) quartz crystals thatwere polished and employed gold electrodes. The QCM sensor wascontained in a bakeable single sensor head (BSH-150, Inficon). TheQCM sensor was sealed with high-temperature epoxy (Epo-TekH21D, Epoxy technology). To prevent deposition on the back-side ofthe QCM sensor, an additional 20 sccm of N2 was flowed through theQCM housing.32
II.II. Ex Situ Film Characterization Using XRR, GIXRD, SE, andXPS. The substrates for the ex situ measurements were boron-dopedSi(100) wafers (p-type, Silicon Valley Microelectronics). The Si waferwas cleaved to produce 2.5 cm by 2.5 cm samples. The samplecleaning procedure involved rinsing with acetone, isopropanol, anddeionized water and then drying with N2 gas.
Ex situ XRR measurements determined the film thicknesses and thedensity. A high-resolution X-ray diffractometer (Bede D1, JordanValley Semiconductors) using Cu Kα (λ = 1.540 Å) X-ray radiationwas used for the XRR measurements. The step size and acquisitiontime for the XRR scans were 10 arcsec and 5 s, respectively. The BedeREFS software package (Bede REFS, Jordan Valley Semiconductors)was used to model the XRR scans to determine the film thickness,surface roughness, and film density. The same X-ray diffractometer wasemployed to study the film structure using GIXRD.
SE was used to obtain the film thicknesses and refractive indices.These measurements employed a spectroscopic ellipsometer (M-2000,J. A. Woollam) with a spectral range from 240−1700 nm and anincidence angle of 75°. The CompleteEASE software package(CompleteEASE, J. A. Woollam) and a Sellmier model were used toanalyze the Ψ and Δ values.34 The Sellmeier model is commonly usedfor optically transparent films such as metal fluoride films.34
XPS was used to determine the film composition.30 The XPSinstrument (PHI 5600) utilized a monochromatic Al Kα X-ray source(1486.6 eV). Depth profiles were obtained using Ar ion sputtering.The AugerScan software package (AugerScan, RBD Instruments) wasemployed to collect the data. The CasaXPS software package(CasaXPS, Casa Software) was used to analyze the data.
III. RESULTS AND DISCUSSIONIII.I. ZrF4 ALD Using Tetrakis(ethylmethylamido)
zirconium (TEMAZ) and HF. Figure 2, panel a shows themass gain determined by QCM measurements during 200cycles of ZrF4 ALD at 150 °C using TEMAZ and HF. Therewas an initial layer of ZrO2 on the QCM sensor grown with 200cycles of ZrO ALD using TEMAZ and H2O as the reactants.35
The ZrF4 ALD cycle was defined by a 1 s dose of TEMAZ, 40 sof N2 purge, a 1 s dose of HF, and 40 s of N2 purge. Thisreaction sequence is designated as (1−40−1−40). Pressuretransients of 20 mTorr and 100 mTorr were produced by theTEMAZ and HF doses, respectively. The ZrF4 ALD growth in
Figure 1. Molecular structures of various metal precursors. The CH2groups are not displayed explicitly.
Figure 2, panel a is linear with a mass gain per cycle (MGPC)of 35.5 ng/(cm2 cycle). In addition, ZrF4 ALD experimentsconducted on initial Al2O3 ALD films showed nearly identicalresults.Figure 2, panel b displays the mass gain during three
sequential ZrF4 ALD cycles in the steady state region at 150 °C.These three cycles were the 98th, 99th, and 100th ZrF4 ALDcycles in Figure 2, panel a. The mass changes coinciding withthe reactant exposures are very distinct. The mass increase afterthe TEMAZ exposure is ΔMTEMAZ = 39.2 ng/(cm2 cycle). Themass change after the HF exposure is ΔMHF = −3.7 ng/(cm2
cycle). The MGPC is 35.5 ng/(cm2 cycle).Figure 3 shows the MGPC and the ΔMTEMAZ/MGPC ratio
during 200 cycles of ZrF4 ALD. The MGPC is 35.5 ng/(cm2
cycle) and consists of constant mass gains of ΔMTEMAZ = 39.2ng/(cm2 cycle) and ΔMHF = −3.7 ng/(cm2 cycle). Except forthe first three ZrF4 ALD cycles, the ΔMTEMAZ/MGPC ratio isconstant at 1.1. The reaction stoichiometry will be determinedlater using this ratio. ZrF4 ALD nucleates almost immediatelyon the initial ZrO2 ALD surface. The MGPC and theΔMTEMAZ/MGPC ratio showed little dependence on the
purge time. The MGPC decreased slightly to ∼33 ng/(cm2
cycle) after extended purge times of 120 s.In situ QCM experiments also examined the self-limiting
behavior of the TEMAZ and HF reactions. The mass gainsduring the TEMAZ and HF exposures at 150 °C are shown inFigure 4, panels a and b, respectively. The previous reactantexposure had reached saturation for each of these exposures. An
Figure 2. (a) Mass gain versus time during 200 ZrF4 ALD cycles withTEMAZ and HF as the reactants on ZrO2 at 150 °C using a reactionsequence of (1−40−1−40). (b) Enlargement of mass gain versus timefor three sequential TEMAZ and HF exposures during ZrF4 ALD inthe steady-state, linear growth regime.
Figure 3. (a) MGPC, ΔMTEMAZ, and ΔMHF and (b) ΔMTEMAZ/MGPC ratio during 200 ZrF4 ALD cycles with TEMAZ and HF as thereactants on ZrO2 at 150 °C.
Figure 4. (a) ΔMTEMAZ versus number of TEMAZ minidoses with theHF exposure fixed at 1.0 s. (b) ΔMHF versus number of HF minidoseswith the TEMAZ exposure fixed at 1.0 s.
exposure time of 0.5 s and a purge time of 40 s defined eachminidose. The TEMAZ and HF reactions both displayed self-limiting behavior. ΔMTEMAZ reached a plateau at ΔMTEMAZ =∼40 ng/(cm2 cycle) after one minidose. Similarly, ΔMHF
leveled off at ΔMHF = ∼ −5 ng/(cm2 cycle) after one minidose.The film growth rate during ZrF4 ALD was also determined
from ex situ XRR and SE measurements. A ZrF4 ALD film wasgrown on a Si wafer using 400 cycles of TEMAZ and HFreaction at 150 °C. XRR and SE measured the thickness of theZrF4 ALD film as 342 and 337 Å, respectively. Thesethicknesses are consistent with growth rates of 0.86 Å/cycleand 0.84 Å/cycle, respectively.The MGPC of 35.5 ng/(cm2 cycle) can be converted to a
growth rate in Å/cycle using the film density. XRR measured aZrF4 film density of 4.1 g/cm3. This XRR density of 4.1 g/cm3
is ∼93% of the bulk density of 4.43 g/cm3 for crystalline ZrF4.36
This density can be used to convert the ZrF4 ALD MGPC of35.5 ng/(cm2 cycle) to a growth rate of 0.87 Å/ cycle. There isgood agreement between the in situ and ex situ measurementsof the ZrF4 ALD growth rate.SE determined a refractive index of n = 1.55 at 589 nm for
the ZrF4 ALD films. The measured refractive index of n = 1.55is consistent with previous measurements of n = 1.56 at 633 nmfor amorphous ZrF4,
37 n = 1.59 for crystalline ZrF4,37 and n =
1.62 for an e-beam grown ZrF4 film at 600 nm.1 The surfaceroughness of the ZrF4 ALD films was measured as 4 Å by XRR.In addition, the ZrF4 ALD films were stable in air. There was nochange in the thickness, film density, and film roughness of theZrF4 films after exposure to atmosphere for one month.III.II. Reaction Mechanism and Stoichiometry for ZrF4
ALD. The surface chemistry for ZrF4 ALD during thesequential TEMAZ and HF exposures can be defined by thefollowing two reactions:
| * +
→ | +−*
x
x
(A) ZrF HF Zr(NEtMe)
ZrF ZrF (NEtMe) HNEtMex x
4 4
4 4 (1)
| +
→ | | * + −−
*
x x
(B) ZrF ZrF (NEtMe) 4HF
ZrF ZrF HF (4 )HNEtMex x4 4
4 4 (2)
The asterisks identify the surface species. The vertical linesseparate the various surface species. HF convertsZrFx(NEtMe)4−x to ZrF4. HF can also adsorb on the ZrF4surface. The number of HF molecules adsorbed on the ZrF4surface relative to the number of ZrF4 species deposited duringone ZrF4 ALD cycle is quantified by the parameter x.Assuming this surface chemistry, the ΔMTEMAZ/MGPC ratio
can be established by
Δ=
ΔΔ + Δ
=−
M MM M
M xMM
MGPCTEMAZ TEMAZ
TEMAZ HF
TEMAZ HNEtMe
ZrF4 (3)
In eq 3, MTEMAZ, MHF, MNEtMe, and MZrF4 are the molar massesof TEMAZ, HF, HNEtMe, and ZrF4, respectively. Theequation for x is
= −Δ
= −Δ
⎡⎣⎢
⎛⎝⎜
⎞⎠⎟⎤⎦⎥
⎡⎣⎢
⎛⎝⎜
⎞⎠⎟⎤⎦⎥
xM
M MM
M
1MGPC
159.1
323.6 167.2MGPC
HNEtMeTEMAZ ZrF4
TEMAZ
TEMAZ
(4)
The QCM measurements at 150 °C shown in Figure 3, panel byield a ΔMTEMAZ/MGPC ratio of 1.1. This ratio of 1.1 producesx = 2.4 from eq 4. This x value of 2.4 indicates that there are 2.4HF molecules adsorbed on the ZrF4 surface after the HFexposure relative to each ZrF4 species deposited during oneZrF4 ALD cycle.The proposed reaction mechanism for ZrF4 ALD in the
steady state regime using TEMAZ and HF as the reactants isshown in Figure 5. In reaction A, Zr(NEtMe)4 molecules react
with HF molecules adsorbed on the ZrF4 surface to yieldZrF2(NEtMe)2 and HNEtMe as reaction products. Figure 5shows two HF molecules per deposited ZrF4 species duringZrF4 ALD. The ZrF2(NEtMe)2 species remain adsorbed on thesurface and HNEtMe is a volatile reaction product. In reactionB, HF converts the adsorbed ZrF2(NEtMe)2 species to ZrF4.HNEtMe is again a volatile reaction product, and additional HFmolecules adsorb to the ZrF4 surface. The adsorption of HF onZrF4 is consistent with the strong Lewis acid nature of ZrF4.
38
III.III. MnF2 ALD Using Bis(ethylcyclopentadienyl)-manganese (Mn(EtCp)2) and HF. The QCM measurementsof mass gain during 200 cycles of MnF2 ALD at 150 °C usingbis(ethylcyclopentadienyl) manganese (Mn(EtCp)2) and HFare displayed in Figure 6, panel a. There was an initial layer ofMnO on the QCM sensor grown with 200 cycles of MnO ALDusing Mn(EtCp)2 and H2O as the reactants.39 The reactionsequence was again (1−40−1−40). A nucleation period wasobserved over the first ∼40 ALD cycles.Figure 6, panel b displays the mass gain during three
sequential MnF2 ALD cycles in the steady state regime at 150°C. These three cycles were the 98th, 99th, and 100th MnF2ALD cycles in Figure 6, panel a. Like the results shown inFigure 2, panel b for ZrF4 ALD, the mass changes are verydistinct. The mass increase after the Mn(EtCp)2 exposure isΔMMn(EtCp)2 = 40.8 ng/(cm2 cycle). The mass loss after the HFexposure is ΔMHF = −25.2 ng/(cm2 cycle). The MGPC is 15.6
Figure 5. Proposed reaction mechanism for ZrF4 ALD using TEMAZand HF as the reactants.
ng/(cm2 cycle). The ΔMMn(EtCp)2/MGPC ratio averaged from100 to 200 cycles of MnF2 ALD is 2.6.The MnF2 ALD growth rate was also derived from ex situ
XRR and SE measurements. A MnF2 film was grown on a Siwafer using 400 cycles of Mn(EtCp)2 and HF reaction at 150°C. XRR and SE analysis then measured MnF2 film thicknessesof 172 and 179 Å, respectively. These thicknesses wereconsistent with growth rates of 0.43 Å/cycle and 0.45 Å/cycle. The XRR measurements obtained a MnF2 density of 3.8g/cm3. This density is ∼95% of the bulk density of 3.98 g/cm3
for crystalline MnF2.36 This density can be used to convert the
MnF2 ALD MGPC of 15.6 ng/(cm2 cycle) to a growth rate of0.41 Å/cycle. This growth rate is in good agreement with the insitu QCM measurements.The surface roughness of the MnF2 ALD films was measured
as 26 Å by XRR. This high surface roughness suggests that theMnF2 ALD film is crystalline. SE determined a refractive indexof n = 1.50 at 589 nm. This measured refractive index isconsistent with the previously measured refractive index of n =1.47−1.50 for MnF2 at 589 nm.34 The MnF2 ALD films werealso stable in air. Like the ZrF4 ALD films, the thickness, film
density, and film roughness of MnF2 films were constant duringstorage for one month in atmosphere.
III.IV. Reaction Mechanism and Stoichiometry forMnF2 ALD. The surface chemistry for MnF2 ALD during thesequential Mn(EtCp)2 and HF exposures can be expressed bythese two reactions:
| * +
→ | +−*
x
x
(A) MnF HF Mn(EtCp)
MnF MnF (EtCp) HCpEtx x
2 2
2 2 (5)
| +
→ | | * + −−
*
x x
(B) MnF MnF (EtCp) 2HF
MnF MnF HF (2 )HCpEtx x2 2
2 2 (6)
The asterisks again indicate the surface species and the verticallines separate the different surface species. HF convertsMnFx(EtCp)2−x to MnF2. HF can also adsorb on the MnF2surface. The number of HF molecules adsorbed on the MnF2surface relative to the number of MnF2 species depositedduring one MnF2 ALD cycle is measured by the parameter x.Given this surface chemistry for MnF2 ALD, the
ΔMMn(EtCp)2/MGPC ratio can be derived from
Δ=
ΔΔ + Δ
=−
M M
M MM xM
M
MGPCMn(EtCp)2 Mn(EtCp)2
Mn(EtCp)2 HF
Mn(EtCp)2 HCpEt
MnF2 (7)
In eq 7, MMn(EtCp)2, MHF, MHCpEt, and MMnF2 are the molarmasses of Mn(EtCp)2, HF, HCpEt, and MnF2, respectively.The equation for x is
= −Δ
= −Δ
⎡⎣⎢⎢
⎛⎝⎜
⎞⎠⎟⎤⎦⎥⎥
⎡⎣⎢⎢
⎛⎝⎜
⎞⎠⎟⎤⎦⎥⎥
xM
M MM
M
1MGPC
194.2
241.2 92.9MGPC
HCpEtMn(EtCp)2 MnF2
Mn(EtCp)2
Mn(EtCp)2
(8)
The QCM measurements at 150 °C yield a ΔMMn(EtCp)2/MGPC ratio of 2.6. This ratio of 2.6 produces x = 0 from eq 8and indicates that there are no HF molecules adsorbed on thesurface relative to each MnF2 species deposited during oneMnF2 ALD cycle. The lack of HF adsorption is in agreementwith MnF2 behaving as a weak Lewis acid with negligibleinteraction between HF and the MnF2 film.Figure 7 displays the proposed reaction mechanism for MnF2
ALD in the steady state regime using Mn(EtCp)2 and HF asthe reactants. In reaction A, Mn(EtCp)2 molecules areadsorbed on the MnF2 surface. In reaction B, HF convertsthe adsorbed Mn(EtCp)2 species to MnF2 and HCpEt is avolatile reaction product. There are no HF molecules remainingon the MnF2 surface after the HF exposure.
III.V. Growth of Additional Metal Fluoride ALD Films.HfF4, MgF2, ZnF2, and additional ZrF4 ALD films were alsodemonstrated using the appropriate metal precursor and HF asthe reactants. In each case, the initial layer on the QCM sensorwas grown using the metal precursor and H2O as the reactants.The reaction sequence for all of the metal fluoride ALDsystems, except ZnF2 ALD, was (1−40−1−40). All the metalfluorides, except ZnF2, showed similar nucleation on theircorresponding metal oxides and on Al2O3 ALD films. Themetal fluoride films were also stable in air. The thickness, filmdensity, and film roughness of films were constant during
Figure 6. (a) Mass gain versus time during 200 MnF2 ALD cycles withMn(EtCp)2 and HF as the reactants on MnO at 150 °C using thereaction sequence of (1−40−1−40). (b) Enlargement of mass gainversus time for three sequential Mn(EtCp)2 and HF exposures duringMnF2 ALD in the steady-state, linear growth regime.
storage in atmosphere for one month. Only the ZnF2 ALD filmwas stored in a desiccator until the ex situ measurementsbecause of its instability in air. Measurements for ZnF2 ALD arepresented in the Supporting Information.Figure 8 shows the QCM measurements of mass gain during
200 cycles of HfF4, ZrF4, and MgF2 ALD at 150 °C. The initial
layer on the QCM sensor was the corresponding metal oxideALD film grown with 200 cycles of ALD using the metalprecursor and H2O as the reactants.35,40,41 Figure 8 reveals thatthe ALD of these three metal fluorides is linear versus thesequential metal precursor and HF exposures except for a briefnucleation period over the first ∼10−12 ALD cycles for ZrF4and MgF2 ALD.Figure 9 shows the mass gain during three sequential ALD
cycles for HfF4, ZrF4, and MgF2 ALD in the steady state regionsat 150 °C. These three cycles were in the linear regimes of theALD growth displayed in Figure 8. The mass gains are verydistinct for each metal fluoride. The mass changes after the
metal precursor and HF exposures are summarized in Table 1.The MGPCs are also given in Table 1. The mass change duringthe metal precursor exposure divided by the MGPC defines theΔMTDMAH/MGPC, ΔMZTB/MGPC, and ΔMMg(EtCp)2/MGPCratios. These ratios are also included in Table 1.The ratios determine the x values that quantify the number
of HF molecules adsorbed on the surface relative to the numberof metal fluoride species deposited during one ALD cycle. Byusing similar equations as given by eqs 4 and 8 for ZrF4 ALDand MnF2 ALD, respectively, x values of 2.2, 2.0, and 0.1 can bedetermined for HfF4, ZrF4, and MgF2 ALD, respectively. The xvalues of 2.2 and 2.0 indicate that there are 2.2 and 2.0 HF
Figure 7. Proposed reaction mechanism for MnF2 ALD usingMn(EtCp)2 and HF as the reactants.
Figure 8. Mass gain versus time during 200 cycles of: (a) HfF4 ALD;(b) ZrF4 ALD; and (c) MgF2 ALD at 150 °C using the reactionsequence of (1−40−1−40).
Figure 9. Enlargement of mass gain versus time for three sequentialmetal precursor and HF exposures in the steady-state, linear growthregime at 150 °C during: (a) HfF4 ALD; (b) ZrF4 ALD; and (c) MgF2ALD.
molecules adsorbed on the HfF4 and ZrF4 surfaces, respectively,relative to each metal fluoride species deposited during oneALD cycle. This behavior is consistent with HfF4 and ZrF4acting as strong Lewis acids. In contrast, the x value of 0.1indicates that there is only 0.1 HF molecule adsorbed on theMgF2 surface relative to each MgF2 deposited during one MgF2ALD cycle. This behavior is in agreement with MgF2 acting as aweak Lewis acid.Metal fluoride ALD films were also grown on Si wafers using
400 cycles of metal precursor and HF at 150 °C. XRR and SEmeasurements of the film thicknesses are consistent withgrowth rates of 0.8, 0.6, and 0.4 Å/cycle for HfF4, ZrF4, andMgF2 ALD, respectively. These growth rates are in goodagreement with the growth rates determined by the MGPCsand film densities. The film densities determined from XRRanalysis are summarized in Table 1. These densities are ∼96%,∼106%, and ∼98% of the bulk densities of HfF4, ZrF4, andMgF2.
36
SE analysis also determined refractive indices of n = 1.55, n =1.62, and n = 1.40 at 589 nm for the HfF4, ZrF4, and MgF2ALD films. The HfF4 refractive index of n = 1.55 at 589 nm isin good agreement with previous measurements of n = 1.57 at600 nm for e-beam evaporated HfF4 film,2 n = 1.59 at 600 nmfor sputtered HfF4 films,42 and n = 1.62 at 600 nm for e-beamgrown HfF4 films.1 The ZrF4 refractive index of n = 1.62 at 589nm is fairly consistent with n = 1.56 measured for amorphousZrF4 at 633 nm,37 n = 1.59 for crystalline ZrF4 at 600 nm,
37 andn = 1.62 at 600 nm for ZrF4 films grown by e-beamevaporation.1 The MgF2 refractive index of n = 1.40 at 589nm is consistent with refractive indices for MgF2 of n = 1.37−1.38 at 589 nm34 and n = 1.38 at 600 nm for MgF2 films grownby sputtering.42
Surface roughnesses were also derived from the XRRanalysis. The surface roughness of the HfF4 ALD films wasmeasured as 5 Å. The surface roughness of the ZrF4 films wasmeasured as 4 Å. The surface roughness of the MgF2 films wasmeasured as 12 Å. This larger surface roughness may resultfrom a higher degree of crystallinity in the MgF2 ALD film.III.VI. Lewis Acid Strength of Metal Fluorides Based
on HF Adsorption. Table 1 summarizes the growth rates,ratios, and x values for the various metal fluorides. The resultsfor AlF3 and LiF from other studies are also included in Table1.30,43 The x values give the number of HF molecules adsorbedon the surface relative to each MFy species deposited duringone MFy ALD cycle. The x values divide the metal fluoridesinto two main groups. High x values of x = 2.0−2.4 areobtained for HfF4 and ZrF4. These surfaces act as strong Lewisacids and adsorb HF. Lower x values of x ≈ 0 are obtained for
MnF2, MgF2, and ZnF2. These surfaces act as weak Lewis acidsand do not adsorb HF.This classification of metal fluorides into two categories
based on their x values is consistent with the Lewis acidproperties of the various metal fluorides. ZrF4 and HfF4 areboth polymeric solids with eight-coordinate metal centers thatare known to form the monoclinic crystal structure.38,44 ZrF4and HfF4 are known to display strong Lewis acid properties.Investigations of ZrF4 and HfF4 complexes with neutral O- andN-donor ligands have revealed that the large metal Zr and Hfcenters can produce up to eight-coordination withoutdifficulty.38 A variety of ligands, such as dimethyl sulfoxideand 2,2′-bipyridyl, were also explored and shown to yield stablecomplexes with ZrF4 and HfF4. These complexes wereconsistent with the Zr and Hf centers acting as Lewis acidsby accepting electron pairs from the ligands.38
HF is a fluorinating agent where the fluorine in HF acts as ananion. The Lewis acidity of ZrF4 and HfF4 can be viewed interms of their ability to adsorb HF by interacting with the F−
anion. Evidence for F− interaction with ZrF4 is obtained fromstudies of molten salt chemistry. In molten salts, ZrF4 forms theZrF6
2− anion by accepting two F− anions by the reaction ZrF4 +2F− → ZrF6
2−.45 In addition, ZrF4 is expected to be a Lewisacid because ZrO2 is known to be an acidic oxide and acts as anoxide ion acceptor.46 HfF4 has also been categorized as a Lewisacid based on its facility to catalyze the isomerization ofmethylpentane to 2,2-dimethyl pentane and n-hexane and thesimultaneous deprotonation of carbonium ion intermedi-ates.47,48
In contrast, MnF2, MgF2, and ZnF2 have lower values of x ≈0 and do not adsorb HF. MnF2, MgF2, and ZnF2 are alldifluorides that form the rutile crystal structure. Thesedifluorides are known to display weak Lewis acid properties.Infrared studies of CO adsorption on MgF2 reveal the presenceof medium or weak Lewis acid sites from magnesium atoms onthe MgF2 surface.49 Pyrrole adsorption experiments also areconsistent with the existence of weak basic sites from thefluorine atoms on the MgF2 surface.49 Similar infraredinvestigations of CO adsorption on ZnF2 reveal that theLewis acidity is even weaker at the Zn2+ sites on ZnF2 surfacescompared with the Lewis acid sites on MgF2 surfaces.
50
The metals in MnF2, MgF2, and ZnF2 have low electro-negativities and are more likely to donate the F− anion thanaccept the F− anion. Viewed in terms of the metal oxides, MnO,MgO, and ZnO are all basic oxides and act as oxide iondonors.46 The corresponding MnF2, MgF2, and ZnF2 metalfluorides would be expected to act as F− ion donors rather thanF− ion acceptors. The low Lewis acidity of MnF2, MgF2, andZnF2 leads to their negligible interaction with HF.
Table 1. Mass Changes, Growth Rates, Ratios, Number of HF per Metal Fluoride, and Lewis Acidity for the Various MetalFluorides
The abilities of AlF3 and LiF to adsorb HF are also consistentwith their Lewis acid strengths. An x value of x = 0.8 wasmeasured earlier during AlF3 ALD studies.30 This x value isconsistent with the Lewis acid nature of AlF3. AlF3 can adsorbHF because AlF3 can act as an F− ion acceptor. Gaseous AlF3 isa very strong Lewis acid.51 Solid AlF3 also has strong Lewis acidsites when AlF3 is in the β-AlF3 phase.
6,52,53 An x value of x =0.1 was also measured during LiF ALD studies. This x value isconsistent with the Lewis base nature of LiF.54 LiF does notadsorb HF because LiF would rather act as a F− ion donor.III.VII. Ex Situ Film Characterization Using SE, XRD,
and XPS. Figure 10 shows the refractive indices of the metal
fluoride ALD films in the spectral range between 240 and 1700nm. Figure 10 includes the refractive indices of AlF3 and LiF.The refractive indices measured at 589 nm are summarized inTable 2. Most of these refractive indices are consistent with thebulk refractive indices reported in the literature as mentionedearlier. The refractive indices of n = 1.55 for the ZrF4 ALD film
and n = 1.55 for the HfF4 ALD film were obtained using theTEMAZ and TDMAH precursors, respectively. ZrF4 ALD filmsgrown using the ZTB precursor have a higher refractive index n= 1.62 attributed to the ∼10% oxygen impurity as discussedbelow.GIXRD analysis indicated that most of the metal fluoride
ALD films have crystalline structures. The metal fluoridesyielding an amorphous film structure were ZnF2 and AlF3. Theamorphous structure of ZrF4 using ZTB as the precursorprobably resulted from the oxygen impurity in the ZrF4 film.ZrF4 using TEMAZ as the precursor yielded a crystallinestructure consistent with the monoclinic phase as given by theJoint Committee on Powder Diffraction Standards (JCPDS)file no. 33−1480. A broad peak at 23° with a full width at half-maximum (FWHM) of 7° corresponds to the overlap of theZrF4 (1̅21) and ZrF4 (2 ̅11) peaks. Another broad peak at 50°was consistent with the ZrF4 (024) peak.HfF4 using TEMAH as the precursor also displayed a
crystalline structure consistent with the monoclinic phase(JCPDS # 79−1040). A very similar broad feature at 23° wasobserved that corresponded to the overlap of the HfF4 (021)and HfF4 (111) peaks. A broad HfF4 (5̅31) peak was alsoobserved at 50°. These broad peaks suggested that ZrF4 andHfF4 have nanocrystalline structure, which leads to widediffraction peaks as predicted by the Scherrer equation.MnF2 film has a crystalline structure consistent with the
tetragonal phase (JCPDS# 88−2143). The MnF2 (110), MnF2(101), MnF2 (211), and MnF2 (220) peaks were located at25.8°, 32.8°, 50.6°, and 53.2°, respectively. MgF2 has a crystalstructure consistent with the tetragonal phase (JCPDS# 72−2231). The MgF2 (110), MgF2 (111), MgF2 (211), and MgF2(301) peaks were located at 27.5°, 40.7°, 53.5°, and 68.4°,respectively. The LiF film has a crystalline structure consistentwith the cubic phase (JCPDS# 04−0857). The LiF (111), LiF(200), and LiF (220) peaks were located at 38.4°, 44.8°, and65.3°, respectively. The crystalline structures of the metalfluoride films are summarized in Table 2.XPS sputter depth-profiling revealed the impurity levels in
the metal fluoride films. The XPS results indicate that most ofthe metal fluoride ALD films have very low levels of impurities.Sputter depth-profiles for the ZrF4 and HfF4 ALD films areshown in Figure 11, panels a and b, respectively. The ZrF4 ALDfilm was deposited using TEMAZ as the metal precursor. Aftersputtering into the depth of the metal fluoride films, HfF4 and
Figure 10. Refractive indices for metal fluoride ALD films grown atwavelengths between 240 and 1700 nm. These refractive indices wereobtained from SE using the Sellmeier model.
Table 2. Densities, Refractive Indices, Crystalline Structures, and Impurities for the Various Metal Fluorides. The JCPDS FileNumbers Are Given for the Crystal Structures
metal fluoride density (g/cm3) refractive index crystal structure impurities by XPS
ZnF2 had no detectable O or C impurities above the XPSdetection limit of ∼0.2 at.%. The MnF2 and MgF2 films hadvery low O impurities of ≤1.0 at.% and no measurable Cimpurities. The ZrF4 film grown using TEMAZ had a larger Cimpurity of 3.4 at.% and a low O impurity of 1.1 at.%. Theimpurities in the metal fluoride ALD films are summarized inTable 2.The ratios between the zirconium and fluorine XPS signals in
Figure 11, panel a and the hafnium and fluorine XPS signals inFigure 11, panel b indicate fluorine deficiencies. Fluorinedeficient metal fluorides have been observed previously in XPSstudies of AlF3 and LiF ALD films.29,30,43 However, Rutherfordbackscattering spectra (RBS) have confirmed that the AlF3ALD films were stoichiometric even though the XPS resultswere showing fluorine deficiencies.29,30 The preferentialsputtering of fluorine may explain the low fluorine XPSsignals.18,19,30,55
The higher levels of oxygen at the surface of the ZrF4 film inFigure 11, panel a may indicate the interaction of the ZrF4 filmwith moisture.56 The ZrF4 ALD film grown using ZTB as themetal precursor had a high O impurity level of ∼10 at.%. Thishigh oxygen impurity level is attributed to some incorporationof the alkoxide ligand from ZTB into the ZrF4 ALD film. In
contrast, the ZrF4 ALD films grown using TEMAZ as the metalprecursor had a lower O impurity of only 1.1 at.%.
IV. CONCLUSIONSVarious metal fluorides were grown using ALD techniques withHF−pyridine as the HF source. The metal fluorides were ZrF4,MnF2, HfF4, MgF2, and ZnF2. The growth of these metalfluorides was monitored using in situ QCM measurements.ZrF4 ALD using tetrakis(ethylmethylamido) zirconium and HFdisplayed a MGPC of 35.5 ng/(cm2 cycle) at 150 °C. ThisMGPC was equivalent to growth rate of 0.9 Å/cycle. MnF2,HfF4, MgF2, ZnF2, and additional ZrF4 were also grown anddisplayed growth rates of 0.4, 0.8, 0.4, 0.7, and 0.6 Å/cycle,respectively, at 150 °C. Nearly all of the ex situ measurementsof the growth rates using XRR and SE analysis were inagreement with the in situ QCM measurements. All of thesemetal fluoride ALD systems displayed self-limiting reactions.The mass changes measured by the QCM after the individual
metal precursor and HF exposures were able to quantify HFadsorption on the metal fluoride surface after the HF reaction.The ZrF4 and HfF4 films adsorbed an average of two HF perdeposited MFy species after the HF reaction. This behavior isconsistent with ZrF4 and HfF4 acting as strong Lewis acids. Incomparison, the MnF2, MgF2, and ZnF2 films did not adsorbHF after the HF reaction. This behavior is consistent withMnF2, MgF2, and ZnF2 behaving as weak Lewis acids.The metal fluoride ALD films displayed refractive indices
that were consistent with previous measurements. XRD studiesrevealed that the majority of the metal fluorides werecrystalline. XPS investigations showed that most of the metalfluorides had high purity. Metal fluoride ALD using HF−pyridine as the HF source will be useful for many applicationsof metal fluorides as optical films, protective coatings for Li ionbattery electrodes and catalysts.
■ ASSOCIATED CONTENT*S Supporting InformationThe Supporting Information is available free of charge on theACS Publications website at DOI: 10.1021/acs.chemma-ter.5b04360.
QCM measurements of ZnF2 ALD using diethylzinc andHF; QCM, XRR, and SE measurements of growth ratefor ZnF2 ALD; surface roughness and refractive index ofZnF2 ALD films (PDF)
■ ACKNOWLEDGMENTSThe National Science Foundation (CHE-1306131) funded thisresearch. The Department of Energy through the DOE-BATTprogram provided additional personnel support for Y.L.
■ REFERENCES(1) Pellicori, S. F.; Colton, E. Fluoride Compounds for IR Coatings.Thin Solid Films 1992, 209, 109−115.(2) Traylor Kruschwitz, J. D.; Pawlewicz, W. T. Optical andDurability Properties of Infrared Transmitting Thin Films. Appl. Opt.1997, 36, 2157−2159.
Figure 11. XPS sputter depth-profiles for (a) ZrF4 ALD films grownusing 400 ALD cycles with TEMAZ as the metal precursor and (b)HfF4 ALD films grown using 400 ALD cycles with TDMAH as themetal precursor.
(3) Niisaka, S.; Saito, T.; Saito, J.; Tanaka, A.; Matsumoto, A.; Otani,M.; Biro, R.; Ouchi, C.; Hasegawa, M.; Suzuki, Y.; Sone, K.Development of Optical Coatings for 157-nm Lithography. I. CoatingMaterials. Appl. Opt. 2002, 41, 3242−3247.(4) Herron, N.; Farneth, W. E. The Design and Synthesis ofHeterogeneous Catalyst Systems. Adv. Mater. 1996, 8, 959−968.(5) Kemnitz, E.; Gross, U.; Rudiger, S.; Shekar, C. S. AmorphousMetal Fluorides with Extraordinary High Surface Areas. Angew. Chem.,Int. Ed. 2003, 42, 4251−4254.(6) Kemnitz, E.; Menz, D. H. Fluorinated Metal Oxides and MetalFluorides as Heterogeneous Catalysts. Prog. Solid State Chem. 1998,26, 97−153.(7) Ding, F.; Xu, W.; Choi, D. W.; Wang, W.; Li, X. L.; Engelhard, M.H.; Chen, X. L.; Yang, Z. G.; Zhang, J. G. Enhanced Performance ofGraphite Anode Materials by AlF3 Coating for Lithium-Ion Batteries. J.Mater. Chem. 2012, 22, 12745−12751.(8) Sun, Y. K.; Lee, M. J.; Yoon, C. S.; Hassoun, J.; Amine, K.;Scrosati, B. The Role of AlF3 Coatings in Improving ElectrochemicalCycling of Li-Enriched Nickel-Manganese Oxide Electrodes for Li-IonBatteries. Adv. Mater. 2012, 24, 1192−1196.(9) Lee, Y.; DuMont, J. W.; George, S. M. Mechanism of ThermalAl2O3 Atomic Layer Etching Using Sequential Reactions withSn(acac)2 and HF. Chem. Mater. 2015, 27, 3648−3657.(10) Lee, Y.; DuMont, J. W.; George, S. M. Atomic Layer Etching ofHfO2 Using Sequential, Self-Limiting Thermal Reactions withSn(acac)2 and HF. ECS J. Solid State Sci. Technol. 2015, 4, N5013−N5022.(11) Lee, Y.; George, S. M. Atomic Layer Etching of Al2O3 UsingSequential, Self-Limiting Thermal Reactions with Sn(acac)2 andHydrogen Fluoride. ACS Nano 2015, 9, 2061−2070.(12) Taki, Y. Film Structure and Optical Constants of Magnetron-Sputtered Fluoride Films for Deep Ultraviolet Lithography. Vacuum2004, 74, 431−435.(13) Iwahori, K.; Furuta, M.; Taki, Y.; Yamamura, T.; Tanaka, A.Optical Properties of Fluoride Thin Films Deposited by RFMagnetron Sputtering. Appl. Opt. 2006, 45, 4598−4602.(14) Heitmann, W. Vacuum Evaporated Films of AluminumFluoride. Thin Solid Films 1970, 5, 61−67.(15) Lee, C. C.; Liu, M. C.; Kaneko, M.; Nakahira, K.; Takano, Y.Characterization of AlF3 Thin Films at 193 nm by ThermalEvaporation. Appl. Opt. 2005, 44, 7333−7338.(16) Barriere, A. S.; Lachter, A. Optical Transitions in DisorderedThin Films of Ionic Compounds MgF2 and AlF3 as a Function ofTheir Conditions of Preparation. Appl. Opt. 1977, 16, 2865−2871.(17) Bridou, F.; Cuniot-Ponsard, M.; Desvignes, J. M.; Richter, M.;Kroth, U.; Gottwald, A. Experimental Determination of OpticalConstants of MgF2 and AlF3 Thin Films in the Vacuum Ultra-VioletWavelength Region (60−124 nm), and its Application to OpticalDesigns. Opt. Commun. 2010, 283, 1351−1358.(18) Schink, H.; Kolbe, J.; Zimmermann, F.; Ristau, D.; Welling, H.″Reactive Ion-Beam-Sputtering of Fluoride Coatings for the UV/VUVRange″. Proc. SPIE 1990, 327−338.(19) Targove, J. D.; Bovard, B. G.; Lingg, L. J.; Angus Macleod, H.Densification of Aluminum Fluoride Thin-Films by Ion-AssistedDeposition. Thin Solid Films 1988, 159, L57−L59.(20) George, S. M. Atomic Layer Deposition: An Overview. Chem.Rev. 2010, 110, 111−131.(21) Ylilammi, M.; Rantaaho, T. Metal Fluoride Thin Films Preparedby Atomic Layer Deposition. J. Electrochem. Soc. 1994, 141, 1278−1284.(22) Pilvi, T.; Hatanpaa, T.; Puukilainen, E.; Arstila, K.; Bischoff, M.;Kaiser, U.; Kaiser, N.; Leskela, M.; Ritala, M. Study of a Novel ALDProcess for Depositing MgF2 Thin Films. J. Mater. Chem. 2007, 17,5077−5083.(23) Pilvi, T.; Puukilainen, E.; Kreissig, U.; Leskela, M.; Ritala, M.Atomic Layer Deposition of MgF2 Thin Films Using TaF5 as a NovelFluorine Source. Chem. Mater. 2008, 20, 5023−5028.
(24) Pilvi, T.; Puukilainen, E.; Arstila, K.; Leskela, M.; Ritala, M.Atomic Layer Deposition of LaF3 Thin Films Using La(thd)3 and TiF4as Precursors. Chem. Vap. Deposition 2008, 14, 85−91.(25) Pilvi, T.; Puukilainen, E.; Munnik, F.; Leskela, M.; Ritala, M.ALD of YF3 Thin Films from TiF4 and Y(thd)3 Precursors. Chem. Vap.Deposition 2009, 15, 27−32.(26) Mantymaki, M.; Hamalainen, J.; Puukilainen, E.; Munnik, F.;Ritala, M.; Leskela, M. Atomic Layer Deposition of LiF Thin Filmsfrom Li(thd) and TiF4 Precursors. Chem. Vap. Deposition 2013, 19,111−116.(27) Hennessy, J.; Jewell, A. D.; Greer, F.; Lee, M. C.; Nikzad, S.Atomic Layer Deposition of Magnesium Fluoride via Bis-(ethylcyclopentadienyl)magnesium and Anhydrous Hydrogen Fluo-ride. J. Vac. Sci. Technol., A 2015, 33, 01A125.(28) Putkonen, M.; Szeghalmi, A.; Pippel, E.; Knez, M. Atomic LayerDeposition of Metal Fluorides through Oxide Chemistry. J. Mater.Chem. 2011, 21, 14461−14465.(29) Lee, Y.; Cavanagh, A. S.; George, S. M. Atomic Layer Depositionof AlF3 Using Trimethylaluminum and Hydrogen Fluoride-Pyridine, 13thInternational Conference on Atomic Layer Deposition (ALD2013),San Diego, California, July 28−31, 2013.(30) Lee, Y.; DuMont, J. W.; Cavanagh, A. S.; George, S. M. AtomicLayer Deposition of AlF3 Using Trimethylaluminum and HydrogenFluoride. J. Phys. Chem. C 2015, 119, 14185−14194.(31) Olah, G. A.; Nojima, M.; Kerekes, I. Synthetic Methods andReactions 0.2. Hydrofluorination of Alkenes, Cyclopropane andAlkynes with (Trialkylamine) Reagents. Synthesis 1973, 1973, 779−780.(32) Elam, J. W.; Groner, M. D.; George, S. M. Viscous Flow Reactorwith Quartz Crystal Microbalance for Thin Film Growth by AtomicLayer Deposition. Rev. Sci. Instrum. 2002, 73, 2981−2987.(33) Lee, Y.; Yoon, B.; Cavanagh, A. S.; George, S. M. MolecularLayer Deposition of Aluminum Alkoxide Polymer Films UsingTrimethylaluminum and Glycidol. Langmuir 2011, 27, 15155−15164.(34) Shannon, R. D.; Shannon, R. C.; Medenbach, O.; Fischer, R. X.Refractive Index and Dispersion of Fluorides and Oxides. J. Phys.Chem. Ref. Data 2002, 31, 931−970.(35) Hausmann, D. M.; Kim, E.; Becker, J.; Gordon, R. G. AtomicLayer Deposition of Hafnium and Zirconium Oxides Using MetalAmide Precursors. Chem. Mater. 2002, 14, 4350−4358.(36) CRC Handbook of Chemistry and Physics, 85th ed.; Lide, D. R.,Ed., CRC Press: Boca Raton, FL, 2005.(37) Almeida, R. M.; Morais, P. J. Preparation and Characterizationof Amorphous ZrF4 Thin Films. J. Non-Cryst. Solids 1995, 184, 93−97.(38) Benjamin, S. L.; Levason, W.; Pugh, D.; Reid, G.; Zhang, W. J.Preparation and Structures of Coordination Complexes of the VeryHard Lewis Acids ZrF4 and HfF4. Dalton Trans. 2012, 41, 12548−12557.(39) Burton, B. B.; Fabreguette, F. H.; George, S. M. Atomic LayerDeposition of MnO Using Bis(ethylcyclopentadienyl) Manganese andH2O. Thin Solid Films 2009, 517, 5658−5665.(40) Burton, B. B.; Goldstein, D. N.; George, S. M. Atomic LayerDeposition of MgO Using Bis(ethylcyclopentadienyl)magnesium andH2O. J. Phys. Chem. C 2009, 113, 1939−1946.(41) Kukli, K.; Ritala, M.; Leskela, M. Low Temperature Depositionof Zirconium Oxide-Based Nanocrystalline Films by Alternate Supplyof Zr[OC(CH3)3]4 and H2O. Chem. Vap. Deposition 2000, 6, 297−302.(42) Martin, P. M.; Olsen, L. C.; Johnston, J. W.; Depoy, D. M.Investigation of Sputtered HfF4 Films and Application to InterferenceFilters for Thermophotovoltaics. Thin Solid Films 2002, 420-421, 8−12.(43) Lee, Y.; Piper, D. M.; Cavanagh, A. S.; Young, M. J.; Lee, S.-H.;George, S. M. Atomic Layer Deposition of Lithium Ion Conducting (AlF3)(LiF)x Alloys Using Trimethylaluminum, Lithium Hexamethyldisilazideand Hydrogen Fluoride-Pyridine, 14th International Conference onAtomic Layer Deposition (ALD2014), Kyoto, Japan, June 15−18,2014.
(44) Papiernik, R.; Mercurio, D.; Frit, B. The Structure of ZirconiumTetrafluoride, Alpha-ZrF4. Acta Crystallogr., Sect. B: Struct. Crystallogr.Cryst. Chem. 1982, 38, 2347−2353.(45) Srikharan, K.; Allen, T. R. Chapter 12 on “Corrosion in MoltenSalts” in Molten Salts Chemistry: From Lab to Applications; Lantelme, F.,Groult, H., Eds.; Elsevier, Inc.: Burlington, MA, 2013.(46) Smith, D. W. An Acidity Scale for Binary Oxides. J. Chem. Educ.1987, 64, 480−482.(47) Kramer, G. M. Ranking Strong Acids via a Selectivity Parameter.1. J. Org. Chem. 1975, 40, 298−302.(48) Kramer, G. M. Ranking Strong Acids via a Selectivity Parameter.2. J. Org. Chem. 1975, 40, 302−307.(49) Wuttke, S.; Vimont, A.; Lavalley, J.-C.; Daturi, M.; Kemnitz, E.Infrared Investigation of the Acid and Basic Properties of a Sol-GelPrepared MgF2. J. Phys. Chem. C 2010, 114, 5113−5120.(50) Guo, Y.; Wuttke, S.; Vimont, A.; Daturi, M.; Lavalley, J. C.;Teinz, K.; Kemnitz, E. Novel Sol-Gel Prepared Zinc Fluoride:Synthesis, Characterisation and Acid-Base Sites Analysis. J. Mater.Chem. 2012, 22, 14587−14593.(51) Christe, K. O.; Dixon, D. A.; McLemore, D.; Wilson, W. W.;Sheehy, J. A.; Boatz, J. A. On a Quantitative Scale for Lewis Acidityand Recent Progress in Polynitrogen Chemistry. J. Fluorine Chem.2000, 101, 151−153.(52) Krahl, T.; Vimont, A.; Eltanany, G.; Daturi, M.; Kemnitz, E.Determination of the Acidity of High Surface AlF3 by IR Spectroscopyof Adsorbed CO Probe Molecules. J. Phys. Chem. C 2007, 111,18317−18325.(53) Wander, A.; Bailey, C. L.; Searle, B. G.; Mukhopadhyay, S.;Harrison, N. M. Identification of Possible Lewis Acid Sites on theBeta-AlF3(100) Surface: An ab initio Total Energy Study. Phys. Chem.Chem. Phys. 2005, 7, 3989−3993.(54) Haupin, W. Chemical and Physical Properties of the Hall-Heroult Electrolyte. In Molten Salt Chemistry: An Introduction andSelected Applications, NATO Science Series C; Mamantov, G., Marassi,R., Eds.; D. Reidel Publishing Company: Dordrecht, Holland, 1987;Vol. 202.(55) Allen, T. H.; Lehan, J. P.; McIntyre, L. C., Jr. Ion BeamSputtered Metal Fluorides. Proc. SPIE 1990, 277−290.(56) Waters, T. N. Some Investigations in the ZirconiumTetrafluoride-Water System. J. Inorg. Nucl. Chem. 1960, 15, 320−328.